How to read a feldspar chemical analysis

A supplier’s analysis sheet is the quickest way to judge whether a feldspar suits your body. Here is how to read one, using our own laboratory results as the example.

What the sheet shows

A whole-rock analysis reports each element as its oxide, in percent by weight. The main oxides add up to roughly 100%. Three extra rows are worth knowing:

  • DL (detection limit): the lowest value the lab can measure reliably.
  • “<0.01”: the oxide is below the detection limit, which in practice means it is negligible.
  • LOI (loss on ignition): the weight lost on heating, from water, carbonates or organic matter. Low LOI means less gas is released during firing.

The four numbers that matter most

1. Na₂O and K₂O: fluxing power

These alkalis decide how strongly the feldspar fluxes. For a sodium feldspar, look at Na₂O first. Pure albite contains about 11.8% Na₂O, so a rough estimate of the albite share is Na₂O ÷ 11.8.

2. Al₂O₃: feldspar content and strength

Alumina usually rises together with Na₂O, because both come from the feldspar mineral itself.

3. Fe₂O₃ and TiO₂: fired colour

These are the colouring oxides. For light-coloured or white bodies, buyers set a maximum for each.

4. SiO₂: free quartz

Silica above what the feldspar itself contains points to free quartz. That is not necessarily a problem, because quartz is part of most tile body recipes anyway.

Worked example: our three grades

CodeNa₂OAl₂O₃SiO₂Fe₂O₃TiO₂LOI≈ albite*
0510.0418.6466.850.890.601.26~85%
037.0414.4176.250.530.060.48~60%
046.5712.5479.210.490.050.45~56%

* A rough estimate (Na₂O ÷ 11.8). It is useful for comparing grades, not a mineralogical measurement.

  • Code 05 is the strongest flux, with the highest Na₂O and Al₂O₃. It also has the most iron and titanium of the three.
  • Codes 03 and 04 contain more free quartz, with very low Fe₂O₃ and TiO₂ and low LOI.
Ask for the analysis with every offer. Better still, test a sample in your own body before you place a large order. We can send you both.

Quick checklist

  1. Is Na₂O (+K₂O) high enough for the fluxing your body needs?
  2. Are Fe₂O₃ and TiO₂ within your colour limits?
  3. Is LOI low?
  4. Do the analysis date and method appear on the sheet?